How to Tell a Gas Bubble from a Shrinkage Void in a Molded Part

Trial Run Defect Guide

How to Tell a Gas Bubble from a Shrinkage Void in a Molded Part

A gas bubble holds trapped gas, while a shrinkage void holds nothing but vacuum. That one difference decides which test you run and which fix you pay for. Warm the spot with a heat gun and watch what the surface does. Gas expands and lifts the skin, sometimes until it pops. A void collapses under air pressure and leaves a sink. This article walks through that test, a cut section, and the fix that follows each result.

What Makes a Gas Bubble Different from a Shrinkage Void?

A gas bubble is a pocket of gas sealed inside the melt. A shrinkage void is an empty space left when the core pulls apart as it cools. Gas gets in during fill, from air, moisture vapor, resin volatiles, or polymer breakdown. A void forms later, during cooling, when the frozen skin holds its shape and the hot core keeps shrinking. The skin cannot move inward, so the core tears open a hollow space inside the wall. That is why a void behaves like an internal sink. Packing can close a void, but packing cannot remove gas that is already sealed in.

Buyers mix the two defects up because both look like a round hole in a clear part. In an opaque part, neither defect shows on the surface at all. The part can pass a visual check and still fail a bend test or a pressure test. That is why the trial report should name the defect type instead of the word bubble alone.

Feature Gas bubble Shrinkage void
Contents Trapped gas Vacuum, no gas
Typical spot End of fill, weld line, rib Center of a thick wall
Heat test Surface swells or pops Surface sinks inward
First fix Dry resin, vent the mold Pack more plastic in

A void and a surface sink share one cause, which is core shrinkage with too little packing. The skin decides which one you see. A soft skin moves inward and shows a sink. A stiff skin holds still, and the core opens a void instead. Our sink mark diagnostic flowchart traces that choice step by step.

Where Does Each Defect Form in the Part?

Location is your first clue, and it costs nothing to record. Mark the defect spot on the part drawing before you change any setting. A gas bubble sits where the melt front traps air. That means the end of fill, a weld line, a deep rib, or a boss with no vent. It can also sit near the gate when gas rides in with the melt stream. A shrinkage void sits in the middle of the thickest wall. Boss centers, rib bases, heavy walls, and thick sections near a gate are the usual spots.

Watch whether the spot moves between shots. A gas trap stays in the same place because the flow path never changes. A moisture bubble jumps around because each shot carries a different amount of vapor. A void stays in the thickest section, but it can grow or shrink as packing changes. If the defect follows the thick wall, treat packing as the prime suspect. If it follows the flow path, look at vents and fill speed first.

A mold flow simulation guide shows what that run can and cannot tell you. Use it to place vents at the last fill area before the trial runs. A simulation will not prove a void, but it will point at the thick section that needs packing. The link below opens our mold flow simulation guide.

How Do You Run the Heat Test?

The heat test is the fastest way to name the defect, and it takes under 15 minutes. Pick a bubble at least 3 mm across on a part molded less than 4 hours ago. Air leaks into an old void through the plastic, so an old part can lie to you. A heat gun is the right tool for this test. A torch runs too hot and can burn the surface before the bubble has time to move.

  1. Warm the area around the bubble with a heat gun until the skin softens.
  2. Keep the gun moving so one spot never scorches.
  3. Watch the surface over the bubble as the plastic turns soft.
  4. Gas makes the skin swell upward, and the bubble may pop.
  5. A void makes the skin fall inward and leave a shallow sink.
  6. Write down the result with the part number, cavity number, shot time, and date.

That written record matters more than the test itself. A trial with no record turns into a fresh argument at the next review. Bozzelli’s heat test for bubbles gives the same steps in full. His rule is plain. Swelling means gas, and collapse means a void.

What Does a Cut Section Show?

Cut the part through the defect when the heat test leaves doubt. Use a fine saw or a sharp blade, then sand the face smooth. A void sits dead center in the thick wall with smooth inner walls. Its surface shows no opening, and the skin above it looks normal. A gas bubble often sits off center, near the surface, a weld line, a rib root, or a blind boss. You may find a small channel that links the bubble back to the surface.

Weigh the suspect part against a known good part from the same cavity. Use the same scale, and record both weights on the trial sheet. A void removes plastic, so the bad part weighs less than the good one. Gas alone changes the weight far less, so a near-normal weight points at gas. Treat this weight check as a screen that points at the cause. A part can carry a small void and still sit close to its normal weight.

A CT scan shows the same hollow space and leaves the part whole. It suits a part you cannot spare, such as a single T1 sample. Cutting stays the faster choice on the trial floor, where a saw sits within reach. Keep one cut sample from each trial and file it with the process sheet.

Which Fix Follows a Gas Bubble?

A gas bubble means gas entered the melt or the cavity, so chase the gas first. Start with the dryer, because wet resin is the most common source. Read the drying log for temperature, time, dew point, and resin lot. Check the resin data sheet next for the drying limits of that grade. The drying guide for hygroscopic resins lists the rules that hold up in production.

If the resin is dry, look at the mold vents next. Clean the parting line vents and the core vents, then check vent depth with pressure sensitive paper. A vent that is blocked or too shallow traps air at the end of fill. Slow the fill near the end so air has time to leave through the vents. A short shot series at 10, 30, 50, 70, and 95 percent fill shows where the flow front folds air in.

Look at the barrel next, because the screw can pump air into the melt. Purge a shot into the air and look for bubbles in the melt. Bubbles in the purge point at the screw or the barrel. Bozzelli lists 1000 to 1500 psi of melt backpressure as one fix for short screws. Cut decompression too, since a long pull can suck air into the nozzle. FCS lays out the same order in its bubble diagnostic sequence. Dryness comes first, then the purge, then the fill pattern.

Take a hypothetical PA66 housing with a bubble at the end of fill. The dryer log shows the correct temperature and time, so moisture drops down the list. A short shot shows the flow front closing around a rib, and the vent at that rib is blocked. Cleaning the vent and slowing the last part of fill clears the bubble. No steel change was needed, and the trial moved on the same day.

Which Fix Follows a Shrinkage Void?

A void means the cavity ran short of plastic as the core cooled, so pack more in. Raise hold pressure and hold time until the gate seals. Check the cushion first, since a screw that bottoms out cannot pack at all. Check the gate next, because a small gate can freeze before the core finishes shrinking. A larger gate, or a gate moved to the thick section, lets packing reach the void. The shrinkage compensation guide shows how mold dimensions are derived from the same shrinkage.

Mold temperature can trade a void for a sink, so use it with care. A hotter mold keeps the skin soft, and the skin then sinks instead of holding a void open. That swap proves the defect was a void, but it does not fix the part. Lower melt temperature can also help, since cooler melt shrinks less in the cavity. Do not chase the void with melt temperature alone. The packing path still has to stay open until the gate seals.

The lasting fix is often a thinner wall. A thick wall freezes at the skin first, and the core has nowhere to pull plastic from. Core out the boss or add ribs for strength instead of piling on wall thickness. Kulkarni makes the same point in his fountain flow and voids piece. There a void reads as an internal sink that packing must fill.

When Do You Change the Mold Instead of the Process?

Steel changes cost time and money, so earn them with two failed process trials. If the defect sits in the same spot after the drying, venting, packing, and gate trials, the mold is the cause. Cut a vent at the last fill area, or add venting to a blind core pin. Move the gate to the thick section so packing reaches the core before the gate seals. Enlarge the gate when the gate seal time is too short to pack the part. Core out a thick boss when the drawing allows it, and add ribs for the lost strength.

Accept the mold only when three shots in a row pass the cut section check. Each part weight must also match the approved first article.